Submit manuscript...
Journal of
eISSN: 2373-4345

Dental Health, Oral Disorders & Therapy

Research Article Volume 10 Issue 4

Assessment of marginal adaptation of lithium disilicate and nanoceramic resin crowns using CAD/CAM system

Vieira Lucas PL, Ávila Gisseli B, Franco Aline BG, Franco Amanda G, Carvalho Geraldo AP, Dias Sérgio C, Ramos Elimário V

Department of Restorative Dentistry, São Leopoldo Mandic Research Institute, Brazil

Correspondence: Amanda Gonçalves Franco, Department of Restorative Dentistry, São Leopoldo Mandic Research Institute, Brazil, Tel 5537999650164

Received: May 31, 2019 | Published: July 24, 2019

Citation: Vieira LPL, Ávila GB, Franco ABG, et al. Assessment of marginal adaptation of lithium disilicate and nanoceramic resin crowns using CAD/CAM system. J Dent Health Oral Disord Ther. 2019;10(4):236?239. DOI: 10.15406/jdhodt.2019.10.00490

Download PDF

Abstract

The aim of this study is to assess the marginal adaptation of different ceramic materials produced by the CEREC system (Sirona, Germany). An analog of the solid abutment Straumann (Straumann, Basel, Switzerland) measuring 5.5mm of height, with platform of 4.8mm, tilt from the axial wall of 6 degrees and chamfer finish line was used as a master model and scanned with an intraoral scanner (CEREC Omnicam). 20 machined crowns were obtained - 10 manufactured from lithium disilicate blocks (IpsE.maxCad, IvoclarVivadent, Liechtenstein, Germany), 10 manufactured from nanoceramic resin blocks (3M ESPE Lava Utimate, USA). The assessment was made using the Replica Technique (RT) and the cementation coating was measured using an optical microscope Mitutoyo (TM 500). Results show a mean marginal disadaptation of lithium disilicate crowns of 78.63µm, which is significantly larger than the one found for nanoceramic resin crowns - 63.15µm. It is possible to conclude that nanoceramic resin crowns have a better marginal adaptation than lithium disilicate ones. Notwithstanding, results found for both groups are within the clinically acceptable values for indirect restorations.

Introduction

In the last years, CAD/CAM technology improved greatly and has provided several applications in dentistry. A variety of drillable materials are available in CAD/CAM for virtually all restoration indications. This technology allows accurate, standardized and fast prosthetic results. One of the main factors for the success of a restoration is marginal adaptation. A large disadaptation between tooth and cement might cause the dissolution of cement, resulting in biofilm accumulation and possibly the occurrence of cavities and/or periodontal disease. Vertical discrepancy at the edge of the restoration is acceptable up to 120µm because it causes smaller cement dissolution.1 The replica and microscopic techniques have been effectively used to assess crown marginal discrepancy.2−5 Ceramic restorations have been widely used in dentistry. Several materials are available in the market, such as lithium disilicate and nanoceramic resin. Lithium disilicate is more resistant and present longer lifespan in clinical use. The nanoceramic resin is a hybrid material that unites the properties of both ceramic and resin.6 Also, materials with different resistances have different abilities to promote adaptation when machined. Materials with larger resistance are less machinable.7 This study compares the marginal adaptation of nanoceramic resin (3M ESPE Lava Utimate, USA) and lithium disilicate (IpsE.maxCad, IvoclarVivadent, Liechtenstein, Germany) crowns, machined in a CAD/CAM system, after the assessment of the replica technique using optical microscopy. 

Proposition

The aim of this study is to compare the marginal adaptation of lithium disilicate (IpsE.maxCad, IvoclarVivadent, Liechtenstein, Germany) and nanoceramic resin (3M ESPE, Lava Ultimate, USA) crowns, machined in a CAD/CAM system, after the assessment of the replica technique using optical microscopy.

Material and methods

This study was approved by the Ethics Committee of the Dentistry School and Research Center São Leopoldo Mandic, under waiver protocol 2015/0488.

An anatomical abutment Straumann® IPS e-max® (Straumann®, Basel, Switzerland) with dimensions of 5.5mm of heigth, platform of 4.8mm, tilt of the axial wall of 6º and chamfer finish was used as master model.

The die was digitized using an intra-oral scanner Omnicam ( Sirona Company, Bensheim, Germany). The crown was simulated using software CAD CEREC 4.4.4 ( Sirona Company, Bensheim, Germany).

A milling machine MCXL ( Sirona Company, Bensheim, Germany) was used to produce 20 actual crowns-10 of lithium disilicate (IpsE.maxCad, IvoclarVivadent, Germany), and 10 of nanoceramic resin (3M ESPE, Lava Utimate, USA) (Figure 1).

Figure 1 Machined crowns.

The replica technique was used to measure the marginal disadaptation.4,5

The assembly abutment-analog was attached to a liner Bioart B2, (Bioart Equipamentos Odontológicos Ltda, São Carlos; Brazil) and inserted into a bipartite acrylic box measuring 2.5cm of width and 2.5cm of height containing, in one half, heavy addition silicone Take 1 Advanced (Kerr Dental, Munich, Germany) for the conformation of the spatial positioning mold.

The crown was cemented to the abutment with light silicone Take 1 Advance (Kerr Dental, Munich, Germany) and repositioned on the heavy silicone mold with a 2kg load on the liner for 2 minutes for the silicone polymerization (Figure 2). The abutment was then removed and the gap created was filled with extra light silicone Take 1 AdvanceMonophase (Kerr Dental, Munich, Germany). The other half of the box was filled with the same heavy silicone and repositioned for the shaping of the abutment replica in fluid silicone.

Figure 2 Cemented crown with fluid silicone.

The replica was covered with medium addition silicone Take 1 Advanced mono/medium (Kerr Dental, Munich, Germany). Following polymerization, it was covered with heavy silicone, forming a replica of the abutment-cement-crown complex. This replica was split in 4 equal parts, and the silicone layer relative to the cementation line was measured in 4 points - mesial, distal, vestibular, and lingual - using a Mitutoyo TM500 (Mitutoyo, Tokyo, Japan) microscope with 30x of magnification (Figure 3). The measurements were submitted to statistical analysis.

Figure 3 Silicone coating on the marginal disadaptation.

Results

The mean values of marginal disadaptation are shown in Tables 1−3.

Nanoceramic resin

Vestibular

Lingual

Mesial

Distal

Mean

Standard deviation

CP1

42

43

56

41

45.50

7.05

CP2

62

50

41

43

49.00

9.49

CP3

89

68

43

74

68.50

19.16

CP4

95

80

83

74

83.00

8.83

CP5

63

71

65

56

63.75

6.18

CP6

87

65

67

63

70.50

11.12

CP7

56

65

82

67

67.50

10.79

CP8

87

73

72

84

79.00

7.62

CP9

56

77

76

45

63.50

15.67

CP10

43

34

45

43

41.25

4.92

Mean

63.15

Standard deviation

13.9

Table 1 Mean marginal disadaptation of the test specimens (CP) in micrometers obtained from nanoceramic resin blocks

Lithium disilicate

Vestibular

Lingual

Mesial

Distal

Mean

Standard deviation

CP1

90

76

83

64

78.25

11.09

CP2

73

66

54

77

67.50

10.08

CP3

76

67

73

84

75.00

7.07

CP4

56

71

73

79

69.75

9.78

CP5

116

98

99

87

100.00

11.97

CP6

89

84

83

88

86.00

2.94

CP7

15

116

95

87

78.25

43.90

CP8

87

98

78

71

83.50

11.68

CP9

77

73

71

69

72.50

3.42

CP10

66

56

88

92

75.50

17.31

Mean

78.63

Standard deviation

9.42

Table 2 Mean marginal disadaptation of the test specimens (CP) in micrometers obtained from lithium disilicate blocks

Group

Mean

Standard deviation

p-value*

Nanoceramic resin

63.15

13.9

0.009

Lithium Dissilicate

78.63

9.42

*Student's t-test for homogeneous variances

Levene's test p=0.228

Table 3 Standard deviation per group

Student's t-test showed that the groups differ with level of significance of 0.05.

Shapiro Wilk's test confirmed normal distribution and Levene's confirmed homogeneity of variances. All statistical tests were conducted on SPSS version 20.0.

Discussion

With the latest technological development, digital solutions have progressively replaced manual processes in all contexts. Dentistry is one of them. New systems and software are routinely being developed and it is up to science to investigate their efficacy. With this in mind, this study aims to contribute to the understanding of CAD/CAM systems application in dentistry.

Restorations with poor marginal adaptation are subjected to cement dissolution and early failure. A marginal disadaptation of more than 120µm show high rate of cement dissolution, thus defining its acceptable limit.1

The use of CAD/CAM technology for the manufacture of indirect restorations has been questioned in terms of its ability to promote good marginal adaptation. Some authors have compared conventional with digital methods.1−5,10−12 Most of these studies failed to find significant differences between the two approaches. However, Colpani et al.,3 found better results using the conventional method of manufacturing of prostheses, and Zarauz et al.5 found the opposite. Nonetheless, both techniques showed satisfactory results. Only a few studies show clinically unacceptable results when using CAD/CAM systems to produce the restorations. One such example is the study by Vojdani et al.,9 that used a combination of conventional and digital methods.

Having established that CAD/CAM systems are capable to promote good marginal adaptation, some studies have engaged in studying the factors influencing the good adaptation of prostheses within the digital workflow.13−15

Some authors (Camargo et al. (2004), Ribeiro et al.,13 Jalali et al.14) found no differences in terms of marginal adaptation when comparing different preparations. On the other hand, Ates &Yesil15 compared shoulder and chamfer finish lines and found better results with the latter. This is the finish line used here. 

Some studies compare marginal adaptation of different CAD/CAM systems. They conclude that CAD/CAM systems, software and parameters within given software may interfere in marginal adaptation.17 Hamza et al.16 used the same CAD/CAM system used here and all results were clinically acceptable.

Some other studies assessed only the system's milling machine.7 They show significant differences in marginal adaptation depending on the type of milling machines, due mainly to the number of axes and thickness of burs. All the authors used, in at least one group, the same milling machine used here and obtained clinically acceptable results.

This study aimed at comparing the marginal adaptation of different materials. This was already done by some authors, with different methodologies.6,7,10,18−20 There is a consensus among them that different materials present different marginal adaptation results, which is in agreement with the results of the present study.

Marginal adaptation is directly linked to the resistance of the material, which interferes in its machinability. Less resistant materials are less machinable.6,7,20,21 This is also in agreement with this study's findings of a marginal adaptation of 63.15µm of the nanoceramic resin group, significantly smaller than the one found for the lithium disilicate group, of 78.63µm. Despite this difference, based on the literature limits, the lithium disilicate group presented an acceptable result.10,19,20−23

Conclusion

Based on the results presented here, it is possible to conclude that:

  1. Nanoceramic resin crowns present better marginal adaptation than lithium disilicate ones.
  2. The materials tested here promote a clinically acceptable marginal adaptation.

Funding

None.

Acknowledgments

None.

Conflicts of interest

The authors declare that there is no conflict of interest.

References

  1. Jacobs MS, Windeler AS. An investigation of dental luting cement solubility as a function of the marginal gap. J Prosthet Dent. 1991;65(3):436–442.
  2. Trifkovic B, Budak I, Todorovic A, et al. Application of Replica Technique and SEM in Accuracy Measurement of Ceramic Crowns. Measurement Science Review. 2012;12(3):90−97.
  3. Colpani JT, Borba M, Della Bona A. Evaluation of marginal and internal fit of ceramic crown copings. Dent Mater. 2013;29(2):174−180.
  4. Berrendero S, Salido MP, Valverde A, et al. Influence of conventional and digital intraoral impressions on the fit of CAD/CAM-fabricated all-ceramic crowns. Clin Oral Investig. 2016;20(9):2403−2410.
  5. Zarauz C, Valverde A, Martinez-Rus F, et al. Clinical evaluation comparing the fit of all-ceramic crowns obtained from silicone and digital intraoral impressions. Clin Oral Investig. 2016;20(4):799−806.
  6. Ruse ND, Sadoun MJ. Resin-composite blocks for dental CAD/CAM applications. J Dent Res. 2014;93(12):1232−1234.
  7. Lebon N, Tapie L, Vennat E, et al. Influence of CAD/CAM tool and material on tool wear and roughness of dental prostheses after milling. J Prosthet Dent. 2015;114(2):236–247.
  8. Ardekani KT, Ahangari AH, Farahi L. Marginal and internal fit of CAD/CAM and slip-cast made zirconia copings. J Dent Res Dent Clin Dent Prospects. 2012 Spring;6(2):42−48.
  9. Vojdani M, Torabi K, Farjood E, et al. Comparison the Marginal and Internal Fit of Metal Copings Cast from Wax Patterns Fabricated by CAD/CAM and Conventional Wax up Techniques. J Dent (Shiraz). 2013;14(3):118−129.
  10. Neves FD, Prado CJ, Prudente MS, et al. Micro-computed tomography evaluation of marginal fit of lithium disilicate crowns fabricated by using chairside CAD/CAM systems or the heat-pressing technique. J Prosthet Dent. 2014;112(5):1134−1140.
  11. Kim JH, Jeong JH, Lee JH, et al. Fit of lithium disilicate crowns fabricated from conventional and digital impressions assessed with micro-CT. J Prosthet Dent. 2016;116(4):551−557.
  12. Memari Y, Mohajerfar M, Armin A, et al. Marginal Adaptation of CAD/CAM All-Ceramic Crowns Made by Different Impression Methods: A Literature Review. J Prosthodont. 2018;28(2):1−9.
  13. Ribeiro VAQ, Sousa RC, Paiva AEM, et al. Evaluation of the marginal fit in copings for full metaloceramic crown with chamfer and beveled shoulder finish line 45º. RFO UPF. 2010;15(3):281−285.
  14. Jalali H, Sadighpour L, Miri A, et al. Comparison of Marginal Fit and Fracture Strength of a CAD/CAM Zirconia Crown with Two Preparation Designs. J Dent (Tehran). 2015;12(12):874−81.
  15. Ates SM, Yesil Duymus Z. Influence of Tooth Preparation Design on Fitting Accuracy of CAD-CAM Based Restorations. J Esthet Restor Dent. 2016;28(4):238−246.
  16. Hamza TA, Ezzat HA, El-Hossary MM, et al. Accuracy of ceramic restorations made with two CAD/CAM systems. J Prosthet Dent. 2013;109(2):83−87.
  17. Shim JS, Lee JS, Lee JY, et al. Effect of software version and parameter settings on the marginal and internal adaptation of crown fabricated with the CAD/CAM system. J Appl Oral Sci. 2015;23(5):515−522.
  18. Della Bona A, Corazza PH, Zhang Y. Characterization of a polymer-infiltrated ceramic-network material. Dent Mater. 2014;30(5):564−569.
  19. De Paula Silveira AC, Chaves SB, Hilgert LA, et al. Marginal and internal fit of CAD-CAM-fabricated composite resin and ceramic crowns scanned by 2 intraoral cameras. J Prosthet Dent. 2017;117(3):386−392.
  20. Chavali R, Nejat AH, Lawson NC. Machinability of CAD-CAM materials. J Prosthet Dent. 2017;118(2):194−199.
  21. Park SH, Yoo YJ, Shin YJ, et al. Marginal and internal fit of nano-composite CAD/CAM restorations. Restor Dent Endod. 2016;41(1):37−43.
  22. Bosch G, Ender A, Mehl A. A 3-dimensional accuracy analysis of chairside CAD/CAM milling processes. J Prosthet Dent. 2014;112(6):1425−1431.
  23. Kirsch C, Ender A, Attin T, et al. Trueness of four different milling procedures used in dental CAD/CAM systems. Clin Oral Investig. 2017;21(2):551−558.
Creative Commons Attribution License

©2019 Vieira, et al. This is an open access article distributed under the terms of the, which permits unrestricted use, distribution, and build upon your work non-commercially.